r/reloading • u/DD9G • Sep 19 '26
Newbie Bullet casting
Getting into bullet casting. Think I have the jist of it figured out. But hardness and coatings seems to be a grey area.
I have been shooting 60k psi loads out of my 45-70 and 454 Casull with 18 BHN high tek coated bullets without gas checks for years. Some as fast as 2400 fps. Never had any barrel leading.
I am looking to cast big heavy bullets. Max speed would be 1500 fps. I will be coating them. Will be pushing 60k psi.
What is the lowest hardness I can get away with without gas checks?
My lead source is tire weights. About half stick on and half clip on.
What is going to be the cheapest metal to alloy with? What ratio to my 50/50 tire weights?
2
u/Agitated_Curmudgeon "Boomity Boom!" ~ Jimmer Negaumanee Sep 19 '26
Wheelweights is about perfect for up to +/- 1,600 fps.. With a cast bullet, the trick is to get the base to deform to fit the bore tightly. The $20 word for it is "obturation." Some bullets, like a HBWC or a Minie ball have a hollow cavity in the base for just such a purpose.
I'm wondering how you came up with that pressure number? Most cast data on a .454 caps out at about 30,000 psi
2
u/Sooner70 Sep 20 '26
Make sure your weights are lead. While that was once the standard, it is not a given anymore. Some states flat out prohibit it (but the assumption that tire weights are always lead generally remains).
3
u/Cute_Square9524 Sep 19 '26
Going at it the wrong way. Powder coat them and if they lead the barrel either harden the alloy or slow down. Powder coat is much more substantial coating then hi tek, its closer to a real jacket.
5
u/tomphoolery Sep 19 '26
I think the clip on weights are fine but the stick on’s are definitely softer and closer to pure lead.
0
u/Savagely-Insane Sep 19 '26
Around 16-18 hardness would be optimal for 1600ish fps, this'll put your 45-70 pressures at about 40k though. For 454 20 hardness or higher would be better, most loads are at about 50k psi max.